Grade and chemical composition | ||||||||||||
Grade | Mass fraction (%) |
| ||||||||||
C | P | S | Mn | Si | Cu | Cr | Mo | Ni | Co | Fe |
| |
≤ |
| |||||||||||
Kovar | 0.03 | 0.020 | 0.020 | 0.5 | 0.30 | 0.20 | 0.20 | 0.20 | 28.5~29.5 | 16.8~17.8 | Balance |
|
tensile strength for strips | |
Status | tensile strength /MPa |
soft | <570 |
hard | >700 |
hardness of strip in deep punching status | ||
status | thickness/mm | Hardness Hv |
deep punching | >2.5 | ≤170 |
≤2.5 | ≤165 |
coefficient of linear expansion | |||||
Grade | heat treating regime | a/(10-6/K) |
| ||
20~300°C | 20~400°C | 20~450°C |
| ||
Kovar | Heat the sample to 900±20°C in hydrogen atmosphere, keep the temperature for one hour, heat again to 1100±20°C and keep the temperature for 15min, then cool to below 200°C at the speed ≤5°C/min and discharge. |
| 4.6~5.2 | 5.1~5.5 |
|
4.3~5.1 | 4.6~5.2 |
|
|
coefficient of expansion | |||||||||
Grade | Average coefficient of expansion a/(10-6/K) |
| |||||||
20~200°C | 20~300°C | 20~400°C | 20~450°C | 20~500°C | 20,600°C | 20~700°C | 20.800°C |
| |
Kovar | 5.9 | 5.3 | 5.1 | 5.3 | 6.2 | 7.8 | 9.2 | 10.2 |
|